Technical
Choosing between SiC and MoSi2.
The choice is set by temperature and atmosphere first, then by how the furnace is wired and how the element is supported. Everything else follows from those three.
| Property | Silicon carbide | MoSi2 |
|---|---|---|
| Practical ceiling, air | 1400 °C continuous | 1700 – 1800 °C |
| Cold resistance | Falls as the element heats | Rises sharply below 400 °C, then falls |
| Ageing | Resistance climbs 5–10% per 1000 h | Stable while the oxide skin holds |
| Surface load | 5 – 8 W/cm² | 1.4 – 2.0 W/cm² |
| Support | Needs support, rods are brittle when hot | Rigid, can be mounted vertically without props |
| Control | Voltage tap or phase-angle control as resistance drifts | Current-limited supply, usually transformer-fed |
| Best fit | Large kilns, low ceiling temperature, cost-sensitive rebuilds | High-temperature sintering, glass, laboratory work |
Atmosphere limits
What each element will and will not take.
Elements fail at the atmosphere before they fail at the temperature. Check this against the process gas before the drawing is approved.
| Atmosphere | Silicon carbide | MoSi2 |
|---|---|---|
| Air / oxidising | Normal service | Normal service; forms a protective silica skin |
| Dry nitrogen, argon | Reduced life, lower ceiling | Short life without an oxide skin; not recommended |
| Hydrogen, CO, cracked ammonia | Not recommended | Not recommended |
| Vacuum | Not recommended | Only above roughly 1000 °C, short cycles |
| Chlorine, sulphur, heavy metal vapour | Not recommended | Not recommended |
Where an atmosphere is unavoidable, the element can sometimes be isolated with a protective tube or a swept gas. Tell us the gas composition and cycle length and we will quote on that basis.
Installation
Four points that decide element life.
Do not mix old and new in one zone(SiC elements)
A new SiC element sits at lower resistance than an aged one in the same circuit. It takes more current and fails first. Replace a zone as a matched set, or re-tap the transformer.
Bring MoSi2 up quickly through 400 °C
A slow climb through the low band lets oxygen attack the surface. Program the ramp to pass through it within a few minutes, then hold at working temperature.
Keep terminals cool and clamped
Terminal ends must sit outside the hot zone, with a clean contact face and a clamp that does not crush the shank. Loose contacts destroy more elements than thermal cycling.
Give the element room to move
SiC expands and sags when hot; MoSi₂ becomes ductile and may deform above 1200°C. Leave adequate clearance, and do not let either element rest against the furnace lining, workpiece, or reactive supports.